Charpy vs Izod: Pendulum Impact Testing of Plastics

Charpy vs Izod: Pendulum Impact Testing of Plastics

How pendulum impact testing works for plastics: Charpy versus Izod geometry, notch types, energy range selection, kJ/m2 versus J/m units, brittle-ductile transition and failure mode interpretation.
2026/11/23
Reading volume: 0

News Details

A tensile test reveals the strength of plastic under gentle pulling force, while an impact test shows what happens when it is struck. The two results are often unrelated: glass-filled nylon can withstand high tensile loads yet still shatter when a housing is dropped, while a softer, weaker grade can absorb the same blow without cracking.

Pendulum impact testing quantifies this difference. A weighted hammer swings from a fixed height, strikes a notched specimen, and continues to a lower height; the energy it loses equals the energy absorbed by the specimen. The principle is a century old, and nearly all disagreements about impact results still come down to its details: geometry, notch type, energy range, and units.

What a Pendulum Impact Test Actually Measures

The raw result is absorbed energy in joules, calculated from the difference between the release angle and the angle the hammer reaches after breaking the specimen. This value includes all the specimen’s resistance mechanisms: elastic deformation, plastic flow, crack initiation at the notch, crack propagation across the remaining ligament, and friction between the broken halves.

Since it is a total value, it is not a material constant like modulus. Impact strength depends on specimen thickness, notch geometry, striker radius, support span, test temperature, and even the direction of molding flow relative to the notch. Two laboratories can test the same pellet and report values 30% apart, both correctly, due to different geometries.

Charpy and Izod: Two Geometries, Two Questions

Both methods use a swinging pendulum to break a notched bar, but they hold the specimen differently, altering the stress state at the notch.

Aspect Charpy Izod
Support Beam supported at both ends Cantilever, clamped at one end
Notch position Faces away from the striker Faces the striker
Impact point Mid-span, opposite the notch Free end, just above the clamp
Typical standards ISO 179, GB/T 1043, ASTM D6110 ISO 180, ASTM D256, GB/T 1843
Reported unit kJ/m² (ISO), J/m or ft-lb/in (ASTM) kJ/m² (ISO), J/m of notch (ASTM)
Where it is preferred European specifications, pipe and profile compounds North American specifications, appliance and automotive parts

Neither method is more accurate. Charpy loads the specimen in three-point bending, typically yielding a lower, more conservative value for ductile materials; Izod places the entire specimen in bending at the clamp, making it more sensitive to surface and edge effects. Due to differing stress fields, values from the two tests cannot be directly converted.

The equipment reflects these geometric differences. A charpy impact tester such as the AT421D series is available in two frame sizes: a 2.9 m/s pendulum with 1, 2, 4, and 5 J weights on a 230 mm center distance, and a 3.8 m/s pendulum with 7.5, 15, 25, and 50 J weights on a 380 mm center distance, both with a 150 to 160-degree release angle, support spacings of 40, 60, 62, and 70 mm or 40, 60, 70, and 95 mm, and a 2 mm striking edge radius. An izod impact tester like the AT422D operates at 3.5 m/s with 2.75, 5.5, 11, and 22 J weights, a 335 mm center distance, and a sharper 0.8 mm striking edge set 22.0 mm above the top of the jaw. These radii and distances are not interchangeable between the two methods, which is why one frame cannot perform both jobs properly.

Notching Decides the Number

A notched specimen concentrates stress at a machined root, so the test measures resistance to crack propagation rather than initiation. Changing the notch alters the result for reasons unrelated to the polymer itself.

  • Notch type. ISO 179 and ISO 180 define type A with a 0.25 mm root radius, type B with 1 mm, and type C with 0.1 mm. A sharper notch creates a higher apparent stress concentration and lower absorbed energy.
  • Notch depth. The remaining ligament under the notch is what ultimately breaks; a deeper notch leaves less material and lowers the result.
  • Notch quality. A machined notch with visible marks or a melted root from a hot knife behaves differently from a clean, single-pass cut.
  • Notch direction. In molded or extruded parts, a notch cut across the flow direction typically yields a different value than one cut along it.

Notch depth measurement is worth automating if throughput is a priority. The AT422D accepts a notch depth measuring device that transmits measured dimensions to the instrument, eliminating the transcription step where most calculation errors originate.

Choosing the Energy Range

Pendulums are not equally accurate across their range. A result is generally considered valid when absorbed energy falls between roughly 10 and 80% of the pendulum’s capacity; below this range, the angle difference is too small to read precisely, and above it, the pendulum decelerates so sharply that the measurement loses meaning.

This is why impact testers come with a set of interchangeable weights rather than a single pendulum, and why a laboratory testing both thin films and glass-filled structural grades requires two frames or a wide weight range. The AT421D covers 1 to 50 J across its two configurations, and the AT422D covers 2.75 to 22 J, sufficient for most rigid plastic and reinforced nylon applications but not for thick composites.

Impact Strength Units Are Not Interchangeable

The most common source of confusion in supplier discussions is the unit.

  • kJ/m², used by ISO 179 and ISO 180, divides absorbed energy by the cross-sectional area under the notch, enabling comparison between specimens of different thicknesses.
  • J/m, used by ASTM D256, divides energy by the notched width only, ignoring thickness; the same material will yield different J/m values at different thicknesses.
  • J, the raw absorbed energy, provides no information about specimen size and should never be used for comparison.

A specification that quotes an impact value without the unit, method, and notch type is not a valid specification. Converting between kJ/m² and J/m requires specimen thickness and remaining ligament width, so any supplier offering a direct conversion factor is oversimplifying something that cannot be simplified.

Temperature and the Brittle-Ductile Transition

Impact energy is strongly temperature-dependent, and for many polymers, the change is abrupt. Below the transition temperature, the material fails by brittle fracture with low absorbed energy; above it, failure is ductile, with yielding, stress whitening, and significantly higher energy. The transition can occur over a range of just a few degrees for some grades, especially those near their glass transition.

Testing only at 23°C provides little insight into a part used in a freezer or under a vehicle hood. A meaningful program measures at several temperatures, conditions specimens in a bath at each temperature, and transfers them to the machine quickly, as a thin specimen warms within seconds of leaving the bath. Hinge performance, drop resistance, and cold-weather cracking all depend on where the service temperature falls relative to this transition.

Reading Failure Mode and Scatter

Absorbed energy alone masks the mechanism. The same value can come from a specimen that yielded and tore or one that fractured cleanly with almost no deformation, and the two have different implications for design.

  • Ductile failure exhibits stress whitening, necking, or a hinged break; energy is high and scatter is typically moderate.
  • Brittle failure shows a flat, shiny fracture surface with no deformation; energy is low and scatter can be large.
  • Mixed failure is common near the transition and produces the widest scatter, which is why at least five, preferably ten, specimens are tested.

Report the failure mode alongside the mean, and treat a high standard deviation as meaningful information rather than noise: it usually indicates a specimen or notch issue, or a material operating at its transition point.

Instrumented Impact: The Curve Behind the Number

An instrumented pendulum records force against time during the few milliseconds of impact, separating crack initiation from propagation. Two materials with the same total energy can differ significantly in how much energy goes into initiating the crack versus propagating it, and this distinction is critical for design against defined flaws. Where an instrumented option is available, it transforms a single value into a curve, at the cost of calibration and analysis effort.

Six Sources of Error in Impact Testing

  1. Wrong energy range. Specimens that barely move the needle, or stop it, yield meaningless values.
  2. Poorly cut notches. Burnt or ragged roots act as unintended stress risers.
  3. Unmeasured specimens. Width and remaining thickness directly enter the calculation.
  4. Uncorrected friction and windage. Older dial machines require manual correction that digital instruments apply automatically; mixing the two introduces systematic offsets.
  5. Slow transfer at low temperature. The specimen reaches room temperature before it is broken.
  6. Too few specimens. Impact scatter is inherent; three results are an anecdote, not a reliable value.

Specifying a Pendulum Impact Tester

Start with the method your customers specify: ISO or ASTM, Charpy or Izod, and the expected thickness range. Confirm the energy range covers your weakest and strongest specimens within the valid band, that support spacing and striking edge match the standard, and that the frame can accommodate the notch types and low-temperature accessories you will need. Verify the calibration process for the pendulum and energy indicator, as an uncalibrated machine will report its own friction losses as material toughness.

Impact results are also evaluated alongside stiffness, heat resistance, and flow data, as a formulation change that improves toughness usually compromises other properties. Laboratories qualifying a compound run impact testers alongside melt flow, thermal, and mechanical instruments from the plastic testing equipment range, so a single trial reports the trade-offs rather than an isolated value.

The practical conclusion is more nuanced than the number suggests. Impact strength is a comparative property measured under a defined geometry, and its value lies in comparing formulations, batches, and suppliers under identical conditions. Used this way, a pendulum test is one of the most effective predictors of field failure available to a plastics laboratory; treated as an absolute material constant, it can be misleading.

Share to:
facebook
line
Whatsapp
Pinterest
Tumblr
Linkedin